Bullseye Reactive Colour Tests

For these tests the main glass I used was Bullseye Reactive Cloud Opal, 000009. It is supposed to react to silver and copper when fired.

The above picture is post-firing. numbered from top left to bottom right, the tests are:

1. Silver leaf on 000009, also half covered by 000009.
2. Silver leaf on 000009
3. Silver leaf between layers of 000009
4. Silver leaf under 000009
5. Bullseye 001116 (Turquoise Blue) between layers of 000009
6. 001116 under 000009
7. 001116 over 0000009
8. New Aquamarine coarse frit on 000009
9. fine and coarse copper wire on 000009
10. coarse copper wire wrapped around 000009
11. fine copper wire wrapped around 000009
12. RW43fp on 000009
13. penny on 000009
14. penny under 000009
15. silver leaf on 001116 with 000009 on top
16. silver leaf on 000009 with 001116 on top
17. RW19 on 000009
18. R05 on 000009
19. RW 215 #2 on 000009
20. RW 219 #2 on 000009
21. RW39hp on 000009

Fired in the mercedes on the following program:

1. 3:00 to 677
2. 3:01 to 804
3. 3:11 @ 804
4. 3:12 to 482
5. 3:40 @ 482
6. 5:10 to 371
7. 5:11 to 20

Fired at 16:00 on Thursday December 10th, out at 15:00 on Friday December 11th.

There really wasn’t much of a reaction in most cases, never with the silver leaf. The copper and copper-bearing glasses each reacted at least a little. The copper turned red, and Bullseye 001116 also turned red.

The most interesting reactions were the following:

This is # 8, New Aquamarine Transparent on 000009. I like the copper halos around each chunk of frit.

Above is RW39 hp, which is copper blue, it turned a dark, rich brown with flecks of bright blue throughout.

Since these were both copper-bearing blues, the differences between the results may have more to do with particle size than with the particular colour used.

The pictures of this firing are in the following album:

Bullseye Reactive Glass Test

Photo-Resist Sand Blasting

In the image above, the top resist blasts away to white, the bottom left blasts away to white, and the bottom right blasts away to black. The photo-resists came back from us ordering them much smaller than expected, so I decided to treat them as tests, to I cut them up and glued them to the differently layered coloured sheet glass that I made.

I did the powder fusing in a previous post in order to sand blast them with photo resist, and the results were pretty good.

Here are the tests I did:
1.1 black powder over red powder on white sheet
1.2 white powder over red powder on black sheet
2.1 black powder on white sheet
2.2 white powder on black sheet
3 blasted into fused sheet, black on steel blue on white.

1.2 (the top right in the picture) was the first one i blasted, I guess the glue hadn’t dried yet, because the resist just blasted right off after about 30 seconds.

I blasted them all at 20psi.

I’m really happy with these results, the detail is good, and would be better with larger images (because the points of resist would be larger and stronger.) In the new year, Amanda and I are planning on exposing out own photo-resist in the print studio. I think I’ll be working this into future projects.

All the photos I have of this are in the following album:

Photo-resist Sandblasting

Powder Fusing

I fused powdered glass to sheet glass (System 96) to have blanks to test some sandblasting techniques. this post is on the fusing firing, future posts will be on the cold working tests.

The above picture is post firing, from top left to bottom right, the tiles are as follows:
1. Thick black powder on white sheet
2. Thin black powder on white sheet
3. Thin black powder on white sheet
4. Thick black powder on white sheet
5. Thin black powder on white sheet
6. Thick white powder on black sheet
7. Thin black powder on white sheet
8. Red powder on black powder on white sheet
9. Red powder on black sheet
10. White powder on red powder on black sheet
11. White powder on black sheet
12. Thin white powder on black sheet
13. Thick white powder on black sheet
14. Red powder on white sheet
15. Red powder on white sheet
16. Black sheet on white powder on black sheet

These were fired in kiln #2, with the following schedule:

1. 3:00 – 538
2. 3:01 – 793
3. 3:31 @ 793
4. 3:32 – 538
5. 4:00 – 516
6. 5:30 – 427
7. 10:00 – 50

The kiln was fired on Monday November 30th, and unloaded on Wednesday December 2nd.

Since the Elements are out on Kiln #2 in the bottom, I built the shelves higher than where the elements are missing. There were two shelves in the Kiln. The powder all fused fully, the texture is not particularly even, it’s a little dappled, and on the ones where there was more than one layer of coloured powder the colour in the middle shows through a little. This might be remedied by sifting thicker layers of colour onto the sheet glass.

The pictures of this firing are in this album:

Powder Fusing

Drawing with glass

I’ve been experimenting with “drawing” on paper with glass. This came out of thinking so much about drawing on glass, I decided to turn it on it’s head and draw with glass instead.

So, this involves paper, water and hot glass. I wet the paper (or not) and take a gather out of the furnace, and drop it on the paper. If the paper catches fire, I drop some water on it to halt the burning.

The variables include how wet the paper is, direction of glass, and how far from the furnace to the paper.

I’ve been experimenting with different weights of watercolour paper. The texture of the heavier ones is lovely with the burn marks, but I quite like how the lighter papers burn through completely in some places, leaving negative spaces in the image. I tried to use some lighter weight papers than watercolour paper, but they pretty much dissolved in the water, and didn’t burn, just sizzled when the glass touched them. Coloured pastel paper is a good weight, but I prefer the plain white of the watercolour paper, it shows off the tonal differences in the burns better.

Don’t worry, the glass in question doesn’t go to waste, I needed frit anyways for kilncasting.

Enamel test firing

So, I’m experimenting with enamels. I though I would start by seeing what colours we had available. I mixed all the low-fire colours with painting medium, gradually adding more medium to the mix to get a range of colour densities.

I painted the enamels on on October 16th, and they didn’t dry before I fired them on the 18th, apparently that’s not a problem for firing, but it meant that since I hadn’t placed them on a perfectly level surface, they ran, and got all mushed up.

The pictures show clear glass tiles with the following colour arrangement:

White, Empire Green
Dark Blue, Leaf Green
Bright Red
Blood Red

Dark Brown, Resolute Blue
Canary Yellow, Green
Best Black, Bright Orange

The black glass tile is painted in the following arrangement:
Empire Green, Dark Blue, Green
Leaf Green, Bright Red, Bright Orange
Blood Red, Dark Brown
Resolute Blue

This test was fired in the mercedes on October 18th, and came out on October 19th.

This was the schedule I used:

1. 0:01 to 575 C
2. 0:20 @ 575 C
3. 0:21 to 515 C
4. 1:50 @ 515 C
5. 5:50 to 427 C
6. 12:00 to 20 C

All the colours fired on at this temperature, except for Best Black, which it turns out I mis-read the label, and it’s a high-fire enamel, so needed temperatures of 650-750C. I’m bad at working in Fahrenheit.

Also, the colour was exceptionally lumpy and uneven. This is because I have never mixed my own paint before this, and I didn’t know I needed to use a palette knife and a muller to get the lumps out. So, Next time I’ll mix the enamels right.

Next step: Silk screening! Decals and direct to glass.

Pictures associated with this firing can be found here:

Enamel Test