Drawing and Process

So, the holidays got in the way of working, as they normally do. I’ve pretty much done nothing but eat and visit for the past two weeks, as one does on the holidays. So, discipline, yeah, I have none. So much for blogging on Wednesdays. That’s obviously something that I should have started after New Years.
I’ve read, in the glut of “how to keep your new years resolutions” things that have been showing up in the past week or so that it is better start one habit at a time, in order to be more likely to actually succeed in building and maintaining it. This is probably good advice, but sometimes I feel like I have so many bad habits that need breaking, and so many things I need to start changing about my life, that I want to start them all now. Probably a bad idea. So, today, I decided that I need to work on developing a habit of drawing. Yes, I’m an artist, and I don’t really draw, or, don’t consider myself very good at it. Mostly, I’m just out of practice, because I don’t do it nearly enough. So today I recycled a lot of paper. Because it’s all about practice, and I’m more likely to open my sketchbook and do something if opening it doesn’t make me feel inadequate by forcing me to look at skills-that-are-crap-when-I’m-rusty. And, really, after a few hours of warming up, I’m not too bad at this drawing thing, and practice will definitely help. So, here’s to creating new habits, like drawing every day, and here’s to tools to help you do it. Like pixelovely’s Figure Drawing Training Tool, which is damn useful for practice.
And to remind me that sometimes process isn’t everything, and doesn’t need to show (so I’m allowed to toss/burn/recycle/feed-to-the-cat my bad drawings) here’s a quote from Annie Dillard’s “The Writing Life” (italics mine):

When you write, you lay out a line of words. The line of words is a miner’s pick, a woodcarver’s gouge, a surgeon’s probe. You wield it, and it digs a path you follow. Soon you find yourself deep in new territory. Is it a dead end, or have you located the real subject? You will know tomorrow, or this time next year.
You make the path boldly and follow it fearfully. You go where the path leads. At the end of the path, you find a box canyon. You hammer out reports, dispatch bulletins. 
The writing has changed, in your hands, and in a twinkling, from an expression of your notions to an epistemological tool. The new place interests you because it is not clear. You attend. In your humility, you lay down the words carefully, watching all the angles. Now the earlier writing looks soft and careless. Process is nothing; erase your tracks. The path is not the work. I hope your tracks have grown over; I hope birds ate the crumbs; I hope you will toss it all and not look back.

Drawing with Frit.

The first non-test firing in the new kiln. Kiln works! Woot!

Nothing complicated. Black powder on Bullseye Tekta.
Before:
After Firing! not much different. except now it won’t blow away!
This programmer works on Rate/Hold, so I’m using that now… and I still like Celsius better.
Firing Program:
Currently Program 1 on Kiln
1. 333C/H to 745C hold 00:10
2. AFAP to 482C hold 1:00
3. 55C/H to 371C hold 00:00
4. AFAP to 21C hold 00:00

Enamel Slumping Test

This is a test to see how the text that I had previously fired onto the sheet glass slumped into a form.
Fired on February 11th in the Mercedes on the following schedule:
1. 1:00 to 125C
2. 4:00 @ 125C
3. 5:00 to 515C
4. 6:00 to 750C
5. 8:30 @ 750C
6. 8:31 to 530C
7. 11:11 @ 530C
8. 16:30 to 400C
9. 19:30 to 20C
I took them out on February 13th.

Pictures of this firing are here:

Enamel Slumping Test

Enamel Firings #2

Yesterday, during my blowslot, I did some tests, firing enamels that had been screen printed directly to sheet glass and firing decals onto previously blown forms.

I set up all of them in the pickup box and sent it up to 560 C, full speed. The sheet glass tests were all set up on a pastorale.

Firing decals onto blown forms:

The decals I made worked alright. I only used the parts that hadn’t smudged completely, and they came off the decal paper alright, except in some cases where drips of the cover coat had gotten around to the reverse side of the paper, which fused the decal to the decal paper in that place.

I put the decals on both the inside of the glass and the outside. They fired on properly in both positions.

Firing enamels on sheet glass on pastorale:

1. a small test, one layer, enamel up.
2. 3 layers, enamels facing up.
3. enameled sides facing each other.

I fired them all in the glory hole until the enamels glowed.

In all the tests I did with the sheet glass, the enamels seem to have fired on properly wether they were exposed to air or not, which I think means that in kiln casting, I wont need to have a separate firing for curing the enamels, and one for fusing.

Frit Tinting Tests

This is a frit-tinting test. All the clear used was System 96.

I tested four colours, Black (G50FP), Crimson (G178FP), Olive Green (G31FP), and Gold Brown (RW215#2) as well as clear.

The three clear test were as follows:

1. 45g clear furnace pellets.
2. 40g clear frit made from blowing furnace.
3. 23g clear powder, very fine. (This is 23g because it was so fluffy that I couldn’t fit more than 23 g in the mold.)

The colour tests were as follows for each colour:

1. 1g colour, 39g clear frit, this is 1/40 colour
2. 2g colour, 38g clear frit, this is 1/20 colour
3. 4g colour, 36g clear frit, this is 1/10 colour
4. 10g colour, 30g clear frit, this is 1/4 colour
5. 16g colour, 24g clear frit, this is 2/5 colour

I mixed the colour and clear by weight, and added some water, shook the mix so that the powder would evenly coat the frit, and poured it into the mold.

Here is a picture of the molds before firing:

These molds were fired in Kiln #5 on the following schedule:

1. 5:00 to 125 C
2. 15:00 to 150 C
3. 22:00 to 650 C
4. 27:00 @ 650 C
5. 27:01 to 875 C
6. 34:00 @ 875 C
7. 34:01 to 520 C
8. 43:00 @ 520 C
9. 61:00 to 390 C
10. 70:00 to 50 C

The kiln was fired at 13:00 on Wednesday December 9th, 2009.

Here are the results:

The black was very strong, it is relatively hard to tell the difference between 10% colour and 40% colour, and almost impossible to tell the difference between 25% and 40%.

In proportions above 25%, the gold brown reduced, showing greens and blues that were quite lovely, but definitely not brown.

The green and red stayed true to colour, and there is noticeable difference between each of the different ratios of colour to clear. When there was less colour, the colouration was less even, most of the pigment concentrating in one place in the test.

For the clear tests, the pellet was almost clean, the frit had quite a few bubbles, and the powder was white and almost opaque.

The pictures associated with this firing can be found here:

Frit Tinting Test

Silk Screening

Yesterday evening, Amanda and finally got into the print studio to do some silk screening.

I had gone in on Monday to shoot a screen, but it didn’t come out very well, so we washed it out (easy!) and re-shot it, this time with both my images and hers.

Both times the screen was shot we used plain laser printer print-outs saturated with vegetable oil to make them transparent. I think that the images that didn’t work weren’t good because they were not dark enough. They were text and line drawings that were quite fine, and they came out clear on the screen where I had traced over them in india ink pen, but not where it was just the computer print out. I think they would have worked out better if they had been on a truly transparent ground, or if they had been darker or bolder lines.

The second screen turned out great, Amanda had a river map, a road map and a suburb map, and I had some text from Pablo Neruda’s “ode to the atom” and my swan images (the ones from the photo sand blasting tests.)

I had already mixed Reusche “Best Black” high-fire enamel on Monday morning, at a ratio of 2:1 decal medium to powder by weight. This time it was smooth, since I first mixed it with a palette knife, and then with a glass muller for 15 minutes.

We did some test prints with normal printing ink, and after finding that we hadn’t completely screwed up the screen, we printed enamel directly onto sheet glass. For each of them the glass was clean, and we flooded the screen before printing. They all went well for a first try at screen printing for both of us, but we could definitely get better detail with more practice.

We also printed the images onto decal paper (which is paper impregnated with gum arabic,) those also worked pretty well.

We also wanted to try to silk screen sandblasting resist. Andy suggested something called “tool dip,” normally used to coating the handles of hand tools, but when each of us asked about it in hardware stores, they staff didn’t know what we were talking about, so we weren’t able to try that, instead we used Weldbond white glue.

Printing glue doesn’t work so well, it seems to degrade the photo resist, so the image was not particularly clear. We thought that we might get a thicker layer of glue if we flooded the screen more times, but that just made the image very smudged. We were also going to try silicone caulking, but decided not to since the screen quality was not so great after the white glue, partially since the silicone we had is quite acidic, so we thought it would just make things worse.

Here are pictures of the results from sand blasting the screen printed glue:

I like them, they aren’t as detailed as the photo resist, of course, but interesting enough. I’m not sure I’d bother to go to the trouble of screen printing it though, glue is a better resist when it is painted on (it stands up to the sandblaster for longer) and the detail isn’t good as we had thought possible.

In the picture above, top left is white powder on black glass, top right is the same, the bottom left is red on white, and the bottom right is red on black.

On Friday afternoon I took everything back into the printing studio to print covercoat on the decals. I’m not even really sure what i did wrong, but the cover coat got everywhere, the coat on the decals was way to thick and ruined the enamels because it made them run. The screen was horrible to clean out, I scrubbed it with mineral spirits for about an hour and the covercoat would come out. Finally, I gave up and pressure washed it out, which worked pretty well.

So, I’ll be firing these on on Sunday during my blow slot, hopefully they work out… I’m not so sure about silk screening, mostly, the results I’ve gotten so far aren’t what I had hoped.